色样及参考技术指标
|
ANOSET <安诺赛特> 毛/涤- 浴法 系列 |
颜色参考样 用量 |
日晒
|
水洗
|
汗渍
|
升华 |
|
0.5 |
2 |
变色 |
涤纶 |
羊毛 |
变色 |
涤纶 |
羊毛 |
变色 |
涤 纶 |
棉 |
|
黄 WP
|
|
|
6-7 |
5 |
4-5 |
5 |
5 |
4-5 |
4-5 |
5 |
3 |
4 |
|
红 WP
|
|
|
6 |
5 |
4 |
4 |
5 |
4 |
4 |
5 |
3 |
4 |
|
大红 WP
|
|
|
5-6 |
5 |
4 |
3-4 |
5 |
4 |
4 |
5 |
3-4 |
4 |
|
兰 WP
|
|
|
5-6 |
5 |
4 |
4 |
5 |
4 |
3-4 |
5 |
3-4 |
4 |
|
灰 WP
|
|
|
6 |
5 |
4-5 |
4-5 |
5 |
4-5 |
4-5 |
5 |
4 |
4-5 |
|
黑 WP
|
|
|
6 |
5 |
4 |
3-4 |
5 |
3-4 |
3-4 |
5 |
2-3 |
3-4 |
|
金黄 WPN
|
|
|
5-6 |
5 |
4-5 |
5 |
5 |
4-5 |
5 |
5 |
4 |
4-5 |
|
红 WPN
|
|
|
6 |
5 |
4 |
4-5 |
5 |
4 |
4 |
5 |
4 |
4-5 |
|
蓝 WPN
|
|
|
6 |
5 |
4-5 |
4-5 |
5 |
4 |
4-5 |
5 |
4 |
5 |
|
藏青 WPN
|
|
|
5-6 |
5 |
4-5 |
4-5 |
5 |
4 |
4 |
5 |
3-4 |
4 |
|
灰 WPN
|
|
|
6 |
5 |
5 |
5 |
5 |
4-5 |
4-5 |
5 |
4 |
4-5 |
|
黑 WPN
|
|
|
6 |
5 |
4-5 |
5 |
5 |
4 |
4 |
5 |
4 |
4-5 |
*注:其中Black WP和Black WPN的用量为2%和4%(owf)。 所有牢度测试均按照以下标准测试方法: light (Daylight) Washing (C06 B2S) 30 minutes at 50 (122ºF) Perspiration (E04) 4 hours at 37 (98ºF); pH 8.0 Sublimation (P01) 30 seconds at 180 (356ºF)
本色卡内所有染料均是通过特定的方法在50/50的毛/涤混纺织物上染色的。
染色方法——ANOSET WP系列染料: 1. 40 染浴制备 X% ANOSET WP 1.0-2.0ml/l 阴离子分散剂或缓冲剂 0.5-2.0% 酸性匀染剂 pH值5.0 用醋酸调整
2. 在40 下搅拌10分钟。 3. 以1-2 /分钟的速度使染液升温到110 。 4. 在110 下保持60分钟。 5. 缓慢降温至70 。 6. 倒掉染液,洗涤样布并按要求后处理。
后处理
染深色时为了达到最佳的效果,推荐使用以下的后处理方法: 0.5-1.5ml/l阴离子精练剂 60 15分钟 然后水洗、干燥
恰当的热处理,如:150 下保温1分钟,可以使纤维上的残留物挥发掉。这样的后处理方法有助于得到较好的日晒牢度,并可去除气味。
染色方法——ANOSET WPN系列染料 1. 40 下制备溶液: X% ANOSET WPN 1.0-2.0ml/l 阴离子分散剂 0.5-2.0ml/l 酸性匀染剂 1.0-2.0ml/l 羊毛保护剂 pH值5.0 用醋酸调整
2. 在40 下搅拌10分钟。 3. 在1-2 /分钟的速度使染液升温到115 。 4. 在115 下保持40分钟。 5. 缓慢降温至70 。 6. 倒掉染液,洗涤样布并按要求后处理。
后处理
染深色时为了达到最佳的效果,推荐使用以下的后处理方法: 0.5-1.5ml/l阴离子精练剂 60 15分钟 然后水洗、干燥
推荐三元色
ANOSET Golden Yellow WPN
ANOSET Red WPN
ANOSET Blue WPN |